Piotr Szajerski1, Marian Zaborski2, Henryk Bem1, Wlodzimierz Baryn2, Edyta Kusiak2.
Abstract
Eight elastomeric composites (NRU, GR1-GR4, NRBG08-NRBG24) containing mixtures of different proportions of heavy metal additives (Bi, W, Gd and Sb) have been synthesized and examined as protective shields. The NRU sample was a pure rubber matrix and served as a reference sample for heavy metal modified composites. Experimental procedure used for evaluation of the composite shields and their attenuation properties was based on the utilization of HPGe spectrometry and analysis of X-ray fluorescence radiation intensity of the heavy metal additives in the following energy ranges for: Sb (20-35 keV), Gd (35-55 keV), W (55-70 keV) and Bi (70-90 keV). The main contributor to the induced X-ray fluorescence radiation within the shield is Bi additive and the intensity of the X-ray radiation generated within the energy range of 70-90 keV strongly depends on its concentration. It was found that decreasing concentration of the Bi fraction from 0.35 (GR samples) to 0.15 (NRBG samples) results in significant lowering Bi X-ray fluorescence radiation within the 70-90 keV energy range. Secondary effect of decreasing Bi concentration was efficient diminishing excitation processes for lower Z heavy metal additives (W, Gd and Sb, GR vs. NRBG samples). As the final quality parameter of the shielding properties for the examined elastomers, dose reduction factor (DRF) coefficients were calculated for each shield. It was found, that the best shielding properties are observed for composites with lower Bi concentration (0.15 vs. 0.35 Bi mass fraction) with only slight further improvement of their parameters (DRF) with increasing of Gd concentration (Gd mass fraction 0.08, 0.16 and 0.24). The most efficient dose reduction composite was found to be NRBG24 elastomer with DRF value 0.47 (53 % dose reduction) for ca. 2 mm and 0.44 g/cm2 layer thickness.Entities:
Keywords: CT; Dose reduction; Elastomer shields; Heavy metal additives; Shielding composites; X-ray florescence radiation
Year: 2014 PMID: 26224969 PMCID: PMC4513903 DOI: 10.1007/s10967-014-2985-5
Source DB: PubMed Journal: J Radioanal Nucl Chem ISSN: 0236-5731 Impact factor: 1.371
Mass fractions of elastomeric composites, phr
| Sample | NR (g) | ZnO (phr) | Sulphur (phr) | MBT (phr) | Stearic acid (phr) | Bi (Bi2O3) (phr) | W (WO3) (phr) | Gd (Gd2O3) (phr) | Sb (Sb2O3) (phr) |
|---|---|---|---|---|---|---|---|---|---|
| NRU | 100 | 5 | 1 | 2 | 2 | – | – | – | – |
| GR1 | 100 | 5 | 1 | 2 | 2 | 62.8 (70.0) | – | – | – |
| GR2 | 100 | 5 | 1 | 2 | 2 | 90.9 (101.3) | 39.0 (49.2) | – | – |
| GR3 | 100 | 5 | 1 | 2 | 2 | 117.1 (130.5) | 50.3 (63.4) | 27.5 (31.7) | – |
| GR4 | 100 | 5 | 1 | 2 | 2 | 132.8 (148.1) | 57.0 (71.9) | 31.2 (36.0) | 12.4 (14.8) |
| NRBG08 | 100 | 5 | 1 | 2 | 2 | 32.0 (35.67) | 32.0 (40.3) | 17.2 (19.8) | 6.6 (7.8) |
| NRBG16 | 100 | 5 | 1 | 2 | 2 | 39.1 (43.6) | 39.1 (49.3) | 41.8 (48.1) | 8.3 (9.9) |
| NRBG24 | 100 | 5 | 1 | 2 | 2 | 50.1 (55.8) | 50.0 (63.0) | 80.7 (93.0) | 10.6 (12.7) |
NR natural rubber, MBT 2-mercaptobenzothiazole, phr parts per hundred rubber
Elemental composition of the Bi–W–Gd–Sb composite shields
| Sample code | Thickness (cm) | Thickness (g/cm2) | Density (g/cm3) | Mass fraction | |||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| H | C | N | O | S | Zn | Sb | Gd | W | Bi | ||||
| NRU | 0.098 | 0.097 | 0.997 | 0.1093 | 0.8176 | 0.0015 | 0.0099 | 0.0252 | 0.0365 | – | – | – | – |
| GR1 | 0.093 | 0.133 | 1.439 | 0.0668 | 0.4996 | 0.0009 | 0.0461 | 0.0154 | 0.0223 | – | – | – | 0.3488 |
| GR2 | 0.105 | 0.0198 | 1.884 | 0.0462 | 0.3452 | 0.0006 | 0.0833 | 0.0106 | 0.0154 | – | – | 0.1498 | 0.3488 |
| GR3 | 0.098 | 0.219 | 2.248 | 0.0358 | 0.2680 | 0.0005 | 0.0949 | 0.0082 | 0.0120 | – | 0.0820 | 0.1498 | 0.3488 |
| GR4 | 0.093 | 0.218 | 2.357 | 0.0316 | 0.2362 | 0.0004 | 0.1009 | 0.0073 | 0.0105 | 0.0325 | 0.0820 | 0.1497 | 0.3489 |
| NRBG08 | 0.115 | 0.191 | 1.658 | 0.0563 | 0.4210 | 0.0008 | 0.0797 | 0.0130 | 0.0188 | 0.0307 | 0.0804 | 0.1497 | 0.1498 |
| NRBG16 | 0.105 | 0.203 | 1.932 | 0.0461 | 0.3447 | 0.0006 | 0.0912 | 0.0106 | 0.0154 | 0.0317 | 0.1601 | 0.1498 | 0.1499 |
| NRBG24 | 0.094 | 0.220 | 2.343 | 0.0359 | 0.2688 | 0.0005 | 0.1025 | 0.0083 | 0.0120 | 0.0318 | 0.2412 | 0.1493 | 0.1496 |
Fig. 1Relative X-ray fluorescence radiation intensities induced in elastomeric composites in a specific energy ranges for: a Sb emission (20–35 keV), b Gd emission (35–55 keV), c W emission (55–70 keV) and d Bi emission (70–90 keV)
Dose reduction factors (DRF) for examined composites
| Composite | Additive(s) |
| DRFa | DRFb |
| DRFa | DRFb |
|---|---|---|---|---|---|---|---|
| NRU | – | 0.097 | 0.92 | 0.92 | 0.194 | 0.91 | 0.91 |
| GR1 | Bi (0.35) | 0.133 | 0.91 | 0.91 | 0.266 | 0.79 | 0.79 |
| GR2 | Bi + W (0.35 + 0.15) | 0.198 | 0.76 | 0.76 | 0.396 | 0.58 | 0.58 |
| GR3 | Bi + W + Gd (0.35 + 0.15 + 0.08) | 0.219 | 0.71 | 0.71 | 0.438 | 0.49 | 0.50 |
| GR4 | Bi + W + Gd + Sb (0.35 + 0.15 + 0.08 + 0.03) | 0.218 | 0.73 | 0.73 | 0.436 | 0.51 | 0.51 |
| NRBG08 | Bi + W + Gd + Sb (0.15 + 0.15 + 0.08 + 0.03) | 0.191 | 0.76 | 0.76 | 0.382 | 0.61 | 0.61 |
| NRBG16 | Bi + W + Gd + Sb (0.15 + 0.15 + 0.16 + 0.03) | 0.203 | 0.72 | 0.72 | 0.406 | 0.54 | 0.54 |
| NRBG24 | Bi + W + Gd + Sb (0.15 + 0.15 + 0.24 + 0.03) | 0.220 | 0.65 | 0.65 | 0.440 | 0.47 | 0.46 |
aX-ray fluorescence radiation of Bi, W, Gd and Sb involved
bOnly for 122.1 and 136.5 keV Co-57 photons
Measured and calculated lead equivalents for investigated elastomeric shields
| Composite | Lead equivalents (in mmPb) for photons energy (keV) | |||||||
|---|---|---|---|---|---|---|---|---|
| 45a | 57a | 79a | 104a | 45b | 57b | 79b | 104b | |
| NRU | 0.0032 | 0.0041 | 0.0042 | 0.0036 | 0.0029 | 0.0040 | 0.0071 | 0.0030 |
| GR1 | 0.0420 | 0.0420 | 0.0370 | 0.0380 | 0.0450 | 0.0460 | 0.0490 | 0.0450 |
| GR2 | 0.0660 | 0.0720 | 0.0760 | 0.0690 | 0.0850 | 0.0870 | 0.1500 | 0.0870 |
| GR3 | 0.1000 | 0.1200 | 0.1200 | 0.1000 | 0.1000 | 0.1300 | 0.2100 | 0.1000 |
| GR4 | 0.1200 | 0.1300 | 0.1400 | 0.1100 | 0.1100 | 0.1400 | 0.2100 | 0.1100 |
| NRBG08 | 0.0620 | 0.0780 | 0.0840 | 0.0630 | 0.0620 | 0.0880 | 0.1500 | 0.0590 |
| NRBG16 | 0.0840 | 0.1200 | 0.1200 | 0.0830 | 0.0720 | 0.1300 | 0.1900 | 0.0700 |
| NRBG24 | 0.1200 | 0.1700 | 0.1800 | 0.1200 | 0.0850 | 0.1700 | 0.2500 | 0.0840 |
aExperimental values
bValues calculated
Fig. 2Dependence of the measured lead equivalents (in mmPb) versus X-ray photons energy for investigated elastomeric shields; relative error of each measurement ±2 %
Fig. 3Correlation between DRF and relative total X-ray fluorescence intensity for high Bi fraction samples (GR series, x Bi = 0.35) and low Bi content (NRBG series, x Bi = 0.15); NRU (reference) sample without heavy metal additives for comparison