Naerin Baek1, Young Kim2, Susan Duncan1, Kristen Leitch1, Sean O'Keefe1.
Abstract
The light-protective effectiveness of titanium dioxide polylactic acid (TiO2 PLA) nanocomposite films (T-PLA) and oleic-acid-modified (OA_TiO2PLA) nanocomposite films was investigated in ready-to-drink (RTD) green tea infusions in oxygen-impermeable glass packaging. The stability of (-)-epigallocatechin gallate (EGCG) was evaluated in RTD green tea infusions in glass packaging covered with PLA (polylactic acid), T-PLA and OT-PLA under fluorescent light during 20 days of storage at 4 °C. Levels of EGCG and color change of RTD green tea infusions were determined. In addition, sensory tests for difference were conducted on green tea infusions in glass packaging without and with complete light protection during 10 days of storage at 4 °C. Of the panelists, 60% noticed sensory differences in the RTD green tea infusion in two different packaging conditions during 10 days of storage under fluorescent light by a triangle test (p < 0.05). During 20 days of storage, levels of EGCG with complete light protection decreased by 10.8% (0.73 mg/mL), and there was a 42.2% loss of EGCG (0.48 mg/mL) in RTD green tea infusions in the glass packaging covered by PLA film. Finally, 3% T-PLA preserved higher levels of EGCG in RTD green tea infusions compared to 1% T-PLA and OT-PLA.Entities:
Keywords: (−)-epigallocatechin gallate (EGCG); fluorescent light; green tea infusion; light protection; polylactic acid (PLA); titanium dioxide (TiO2)
Year: 2021 PMID: 33805540 PMCID: PMC8066687 DOI: 10.3390/foods10040723
Source DB: PubMed Journal: Foods ISSN: 2304-8158
Thickness (mean ± standard deviation) of Polylactic Acid (PLA), 3% TiO2 PLA nanocomposite films (T-PLA), 1% T-PLA, 3% oleic-acid-modified OA_TiO2PLA nanocomposite films (OT-PLA) and 1% OT-PLA nanocomposite films covered the glass bottles (n = 6).
| Sample ( | Mean (μm) ± Std. Dev. |
|---|---|
| PLA | 70.6 ± 15.1 |
| 3% T-PLA | 62.2 ± 8.06 |
| 1% T-PLA | 61.1 ± 9.61 |
| 3% OT-PLA | 66.7 ± 4.7 |
| 1% OT-PLA | 62.2 ± 10.3 |
Changes of EGCG (mg/mL) in ready-to-drink green tea infusions stored in light-blocking (LB) glass packaging and clear glass light-exposed (EX) packaging under light exposure at 4 °C during 10 days of storage. The concentration (mg/mL) of LB and EX is expressed as means (n = 2). A significant difference between the two treatments is expressed with different superscript letters (a or b) next to the data (p < 0.05).
| Storage Time | EGCG (mg/mL) | |
|---|---|---|
| LB | EX | |
| 0 days | 0.51 | 0.51 |
| 10 days | 0.47 a | 0.43 b |
Figure 1(−)-Epigallocatechin gallate concentrations in green tea infusions in glass bottles covered by foil, PLA, 3% T-PLA, 1% T-PLA, 3% OT-PLA and 1% OT-PLA nanocomposite films at Days 0, 10 and 20 under fluorescent light illumination at 4 °C. Significant differences between the samples are expressed with different superscript letters above the data by Tukey’s analysis with p < 0.05. Bars represent the means of three replicates, and significant differences (p < 0.05) are presented by different letters.
Figure 2The light spectrum from the fluorescent bulbs was measured at 2393 lux by using a Upertek MK350S.
Color changes (mean ± standard deviation) in L*value (L*: 0 = black, 100 = white), a- and b-values of ready-to-drink (RTD) green tea in the glass bottles covered by foil, PLA, 3% T-PLA, 1% T-PLA, 3% OT-PLA and 1% OT-PLA nanocomposite films during storage of 0 and 20 days at 4 °C under fluorescent light. Different letters next to the data indicate statistical differences between L, a- and b-values of the color at p < 0.05.
| L-values | ||||||
| Sample | Foil | PLA | 3% T-PLA | 1% T-PLA | 3% OT-PLA | 1% OT-PLA |
| 0 days | 92 ± 0.8 | 92 ± 0.8 | 92 ± 0.8 | 92 ± 0.8 | 92 ± 0.8 | 92 ± 0.8 |
| 20 days | 97 ± 1 a | 97 ± 0.1 a | 95 ± 0.1 bc | 96 ± 0.1 ab | 96 ± 0.1 ab | 94 ± 0.4 c |
| a-values | ||||||
| Sample | Foil | PLA | 3% T-PLA | 1% T-PLA | 3% OT-PLA | 1% OT-PLA |
| 0 days | 0.36 ± 1 | 0.36 ± 1 | 0.36 ± 1 | 0.36 ± 1 | 0.36 ± 1 | 0.36 ± 1 |
| 20 days | −1.38 ± 0.1 c | −0.46 ± 0.4 a | −1.14 ± 0.4 bc | −1.03 ± 0.2 bc | −0.72 ± 0.2 ab | −0.69 ± 0.3 ab |
| b-values | ||||||
| Sample | Foil | PLA | 3% T-PLA | 1% T-PLA | 3% OT-PLA | 1% OT-PLA |
| 0 days | 3.8 ± 0.2 | 3.8 ± 0.2 | 3.8 ± 0.2 | 3.8 ± 0.2 | 3.8 ± 0.2 | 3.8 ± 0.2 |
| 20 days | 2.4 ± 0.1 a | −2.0 ± 0.1 c | −1.0 ± 0.2 b | −1.3 ± 0.2 bc | −1.9 ± 0.1 c | −1.3 ± 0.3 bc |