| Literature DB >> 32325787 |
Ana P Piedade1, Liliana Cangueiro2.
Abstract
This study concerns the evaluation of the coefficient of friction, at different temperatures, of amorphous carbon thin films, depoEntities:
Keywords: 2D carbon thin films; nanocrystalline copper coating; sp1 carbon bonds; zero coefficient of friction
Year: 2020 PMID: 32325787 PMCID: PMC7222008 DOI: 10.3390/nano10040780
Source DB: PubMed Journal: Nanomaterials (Basel) ISSN: 2079-4991 Impact factor: 5.076
Designation, deposition parameters, and thickness of copper and carbon deposited thin films.
| Designation | Deposition Parameters | Thickness (nm) | ||
|---|---|---|---|---|
| Ddep Cu (W·mm−2) | Ddep C (W·mm−2) | Time (s) | ||
| Cu | 3.2 × 10−2 | 0 | 600 | 600 |
| C15 | 0 | 2.5 × 10−2 | 300 | 15 |
| C60 | 0 | 2.5 × 10−2 | 1800 | 60 |
| C100 | 0 | 2.5 × 10−2 | 3600 | 100 |
Figure 1Scanning electron microscopy (SEM) micrographs of C thin films (a) C15, (b) C60, (c) C100. Surface morphology onto Si substrate and cross-section onto Cu thin film.
Figure 2Atomic force microscopy (AFM) surface topographic images of (a) C15, (b) C60 and (c) C100 thin films deposited onto Cu coating. (d) 2D profile of the line highlighted in image (a).
Figure 3Deconvolution of the high resolution spectra of surface Cu-C15: (a) C1s, indicating only the presence of carbyne (sp1) and graphene-like (sp2) hybridized bonds, as well as the presence of C–O bonds; (b) O1s, showing that oxygen is manly bounded to carbon.
X-ray photoelectron spectroscopy (XPS) data from the deconvolution of C1s high-resolution spectra of carbon coatings.
| C Bonds | Surface | |||
|---|---|---|---|---|
| C15 | C60 | C100 | ||
| sp1 | Peak Position (eV) | 282.6 | 282.4 | n.d. |
| Concentration (%) | 35.7 | 5.2 | n.d. | |
| FWHM (eV) | 1.4 | 1.9 | n.d. | |
| sp2 | Peak Position (eV) | 284.1 | 284.2 | 284.2 |
| Concentration (%) | 57.2 | 60.3 | 47.4 | |
| FWHM (eV) | 1.9 | 1.3 | 1.3 | |
| sp3 | Peak Position (eV) | n.d. | 284.9 | 285.0 |
| Concentration (%) | n.d. | 18.0 | 34.0 | |
| FWHM (eV) | n.d. | 1.7 | 1.4 | |
| C–O | Peak Position (eV) | 286.1 | 286.3 | 286.2 |
| Concentration (%) | 7.1 | 9.3 | 15.2 | |
| FWHM (eV) | 2.0 | 1.7 | 2.2 | |
| O–C–O | Peak Position (eV) | 287.6 | 287.5 | n.d. |
| Concentration (%) | 3.4 | 7.2 | n.d. | |
| FWHM (eV) | 2.0 | 1.7 | n.d. | |
n.d.—not determined by the fitting process.
Figure 4Micro-raman spectra of carbon thin films: (a) C15, (b) C60, and (c) C100.
Relative intensity ratio of Raman peaks and G peak position of carbon thin films.
| Surface | G Peak Position | Intensity Ratios | ||
|---|---|---|---|---|
|
|
|
| ||
| C15 | 1574 | 0.57 | 0.30 | 3.0 |
| C60 | 1551 | 0.62 | 0.25 | 3.3 |
| C100 | 1531 | 0.37 | 0.04 | 5.2 |
Figure 5Structural characterization of the Cu thin film: (a) X-ray diffractogram, at room temperature and after 24h at 200 °C; (b) Transmission electron microscopy (TEM) bright field image of the as-deposited coating; (c) TEM bright field image after 2h at 200 °C; (d) TEM bright field image after 24h at 200 °C; (e) electron diffraction pattern of the area showed in (a).
Hardness (H) and Young’s modulus (E) of the deposited surfaces and bulk copper.
| Surface | ||
|---|---|---|
| Cu | 2.64 ± 0.07 | 168 ± 10 |
| C15 | 2.75 ± 0.26 | 164 ± 13 |
| C60 | 2.86 ± 0.07 | 126 ± 5 |
| C100 | 2.95 ± 0.10 | 101 ± 2 |
| Bulk Copper | 1.91 ± 0.09 | 144 ± 19 |
| Bulk Copper (1 N) | 0.99 ± 0.02 | - |
Figure 6Coefficient of friction of bulk copper and Cu thin film at different loads and different temperatures.
Figure 7Coefficient of friction, optical macrographs, and micro-Raman characterization of the wear tracks of Cu-C15 after tribology tests, with 2 N load at different temperatures (bar = 500 μm).
Figure 8Coefficient of friction, optical macrographs, and micro-Raman characterization of the wear tracks of Cu-C60 after 500 sliding cycles, with 2 N load, at different temperatures (bar = 500 μm).
Figure 9Coefficient of friction, optical macrographs, and micro-Raman characterization of the wear tracks of Cu-C100 after the tribology tests, with 2 N load at different temperatures (bar = 500 μm).
Figure 10Optical macrographs of the steel balls after the tribology tests, at 200 °C, with the carbon coatings: (a) Cu-C15, 500 cycles; (b) Cu-C15, 150 cycles; (c) Cu-C60, 500 cycles; (d) Cu-C100, 500 cycles (bar = 200 μm).