| Literature DB >> 29360772 |
Lorenzo Massimo Polgar1,2, Francesco Criscitiello3, Machiel van Essen4, Rodrigo Araya-Hermosilla4, Nicola Migliore5, Mattia Lenti6,7, Patrizio Raffa8, Francesco Picchioni9,10, Andrea Pucci11.
Abstract
Conductive rubber nanocomposites were prepared by dispersing conductive nanotubes (CNT) in thermoreversibly cross-linkedEntities:
Keywords: Joule effect; crack-healing; rubber nanocomposite; strain sensor; thermoreversible cross-linking
Year: 2018 PMID: 29360772 PMCID: PMC5853691 DOI: 10.3390/nano8020058
Source DB: PubMed Journal: Nanomaterials (Basel) ISSN: 2079-4991 Impact factor: 5.076
Figure 1Furan functionalization and bismaleimide (BM) cross-linking of EPM-g-furan and the integration of CNT fillers via covalent interactions in the thermoreversibly cross-linked network of the nanocomposite.
Figure 2Schematic illustration of the circuit used for determining the sample resistance under strain.
Figure 3Illustration of the practical procedure to perform welding tests using a home-made device and exposing the freshly cut sample bar to a source potential (I).
Composition and properties of a homologous series of rubber/carbon nanotube composites.
| EPM * Rubber | CNT (wt %) | BM † (g) | TGA ‡ Residue at 600 °C (%) | Gel Content (%) | Cross-Link Density (10−4 mol/mL) | CNT (wt %) |
|---|---|---|---|---|---|---|
| EPM-g-MA | - | - | 0.0 | 0 | - | - |
| 3.023 g EPM-g-MA | 2.4 | - | 1.7 | 25 | 0.23 | 2.4 |
| 3.047 g EPM-g-MA | 3.5 | - | 9.4 | 55 | 0.64 | 3.5 |
| EPM-g-furan | - | - | 0.0 | 0 | - | - |
| 3.019 g EPM-g-furan | 2.4 | - | 1.6 | 68 | 0.75 | 2.4 |
| 3.007 g EPM-g-furan | 3.4 | - | 9.5 | 82 | 0.95 | 3.4 |
| 3.010 g EPM-g-furan | - | - | 0.0 | 93 | 2.1 | - |
| 3.012 g EPM-g-furan | 2.4 | - | 1.5 | 95 | 5.2 | 2.4 |
| 3.036 g EPM-g-furan | 4.0 | 0.114 | 4.3 | 96 | 3.6 | 4.0 |
| 3.024 g EPM-g-furan | 4.8 | 0.114 | 4.1 | 98 | 4.0 | 4.8 |
| 3.146 g EPM-g-furan | 5.6 | 0.118 | 10.1 | 99 | 4.7 | 5.6 |
| 3.028 g EPM-g-furan | 6.5 | 0.113 | 7.7 | 99 | 6.3 | 6.5 |
* Ethylene propylene rubber. † Bismaleimide. ‡ Thermographic analysis.
Figure 4Scanning electron microscopy (SEM) micrograph of EPM-g-furan/CNT nanocomposites with (a) 7 wt % and (b) 10 wt % CNT loading.
Figure 5Median stress-strain curves of (BM cross-linked) EPM-g-furan/CNT nanocomposites with various CNT loading before (solid lines) and after reprocessing (dashed lines).
Figure 6Cyclic tensile test results of CNT nanocomposites with (A) EPM-g-MA, (B)EPM-g-furan and (C) BM cross-linked EPM-g-furan (right) containing 5 and 10 wt % of CNT.
Tensile strength and elongation at break of EPM-g-MA, EPM-g-furan, BM cross-linked EPM-g-furan and reprocessed BM cross-linked EPM-g-furan with different amounts of (modified) CNT. Typical standard deviations ±10% and ±15–20% of the original value of the tensile strength (Tb) and elongation at break (Eb), respectively.
| Filler Loading (wt %) | EPM-g-MA | EPM-g-Furan | BM Cross-Linked EPM-g-Furan | Reprocessed, Cross-Linked EPM-g-Furan | |||||
|---|---|---|---|---|---|---|---|---|---|
| No CNT | 1.2 | 950 | 1.3 | 750 | 2.2 | 210 | 1.7 | 190 | |
| CNT | 2 | 2.5 | 250 | 2.5 | 250 | 3.1 | 200 | 2.9 | 190 |
| 5 | 3.7 | 200 | 3.8 | 180 | 5.2 | 140 | 5 | 130 | |
| 10 | 5 | 130 | 5.1 | 130 | 7 | 80 | 6.5 | 90 | |
| modified CNT | 2 | 2.5 | 240 | 2.6 | 220 | 3.0 | 210 | 2.9 | 200 |
| 5 | 5.3 | 180 | 5.7 | 150 | 6.3 | 120 | 6.2 | 110 | |
| 10 | 7.2 | 110 | 7.5 | 100 | 7.8 | 100 | 7.5 | 90 | |
Figure A1Comparison between the FT-IR spectra of pristine carbon nanotubes (black) and functionalized carbon nanotubes (red).
Figure A2(a) TGA analysis under nitrogen atmosphere of pristine MWCNTs (blue) and two different batches of MWCNT -FAs (red and black) FA obtained under the same conditions of functionalization and (b) the first derivative of these curves.
Figure A3(a) XPS spectra of non-functionalized (black/down) and FFA functionalized (blue/up) CNT and (b) the first derivative of those spectra in the region relative to the peak photoemission on the N 1s orbital at around 400 eV. The signal was analyzed by deconvolution operated by the instrument software.
Figure A4SEM images at of a FFA functionalized CNT, with an increase in magnification in going from (a) to (b), display that both the length (500 nm) and the diameter (20 nm) are still in agreement with the dimensions assessed by the producer.
Figure 7Conductivity of nanocomposites of EPM-g-MA (black), EPM-g-furan (red) or BM cross-linked EPM-g-furan (blue) with CNT as a function of the CNT loading. The error bars indicate ± 2 standard deviations.
Figure 8Electrical resistivity versus time over 5 cycles of 10% strain on BM cross-linked EPM-g-furan samples containing (a) 10 wt % and (b) 5 wt % of CNT. Each red line indicates the end of one cycle of strain.
Figure 9Resistance variation as a function of elongation for sample bars of BM cross-linked EPM-g-furan nanocomposites at around their percolation threshold (containing 5 wt % of CNT) for up to three cycles of elongation to 100%. The error bars indicate ± 2 standard deviations.
Figure 10Thermal image of BM cross-linked EPM-g-furan containing 5wt % of CNT at 7 V and ~50 mA.
Figure 11Crack-healing by welding of nancomposites of BM cross-linked EPM-g-furan with 5 wt % CNT performed by exposing the sample materials to a potential source of 7 V and 0.05. (a) A macroscopic scratch before and after 30 min of crack-healing by welding and (b) the tensile test of a nanocomposite sample bar before and after re-attaching the broken parts by crack-healing by welding for 90 min.
The percentage of each element present in the non-functionalized and FFA functionalized CNT. Each analysis was repeated on three different portions of the sample analyzed.
| C | O | N | |
|---|---|---|---|
| non-functionalized CNT | 91 | 9 | 0 |
| 90 | 10 | 0 | |
| 89 | 11 | 0 | |
| FFA functionalized CNT | 93 | 4.9 | 2.0 |
| 93 | 5.1 | 1.6 | |
| 93 | 5.3 | 1.6 |